J-3760
repairRepair- Line
- LN-12
- Station
- 2256+00
- Weld date
- 2026-06-11
- Spec
- 24" × 0.375"
34.09360, -104.45560
No open cross-check alerts on this joint.
Welder passes
- RootDitch sideMarcus Cole RC-118
Jun 11, 2026, 8:35 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- RootWorking sideMarcus Cole RC-118
Jun 11, 2026, 8:35 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- Hot PassWorking sideTravis Nolan RC-307
Jun 11, 2026, 9:10 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- Hot PassDitch sideTy Maldonado RC-552
Jun 11, 2026, 9:10 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- FillWorking sideKelly Boudreaux RC-350
Jun 11, 2026, 9:45 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- FillDitch sideSam Whitfield RC-388
Jun 11, 2026, 9:45 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- CapWorking sideSam Whitfield RC-388
Jun 11, 2026, 10:20 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- CapDitch sideCody Latham RC-165
Jun 11, 2026, 10:20 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- RepairWorking sideJesse Karr RC-455
Jun 11, 2026, 10:30 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
NDT results
- RTRepair
Jun 11, 2026, 8:00 PM · D. Halloran (ASNT II)
Fit-up gap out of tolerance (charged to spread, not welder)
Not charged to a welder.
Repairable indication — grind and re-weld authorized.
RT film map — clock position3 indications12123456789101112- IFIncomplete fusion1:29–1:40 · 1.18" · d 0.02"IF exceeds API 1104 acceptance limits — charged for re-work.
- PORPorosity9:14–9:15 · 0.12" · d 0.06"Within acceptance limits.
- UCUndercut11:54–11:59 · 0.51" · d 0.01"Within acceptance limits.
Visual inspection (CWI)
API 1104
Coating inspection
No coating inspection recorded for this joint.