J-3640
repairRepair- Line
- LN-12
- Station
- 2184+00
- Weld date
- 2026-06-10
- Spec
- 24" × 0.375"
34.02040, -104.38840
No open cross-check alerts on this joint.
Welder passes
- RootDitch sideOdell Rains RC-121
Jun 10, 2026, 8:35 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- RootWorking sideWeston Trahan RC-133
Jun 10, 2026, 8:35 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- Hot PassWorking sideJunior Escamilla RC-158
Jun 10, 2026, 9:10 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- Hot PassDitch sideHector Ruiz RC-528
Jun 10, 2026, 9:10 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- FillWorking sideKelly Boudreaux RC-350
Jun 10, 2026, 9:45 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- FillDitch sideSam Whitfield RC-388
Jun 10, 2026, 9:45 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- CapDitch sideKelly Boudreaux RC-350
Jun 10, 2026, 10:20 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- CapWorking sideSam Whitfield RC-388
Jun 10, 2026, 10:20 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- RepairWorking sideJesse Karr RC-455
Jun 10, 2026, 10:30 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
NDT results
- RTRepair
Jun 10, 2026, 8:00 PM · D. Halloran (ASNT II)
Hot pass — incomplete fusion charged to the hot pass welder
Charged to Hector Ruiz (RC-528) — counts as a strike under the 3-repair rule.
Repairable indication — grind and re-weld authorized.
RT film map — clock position2 indications12123456789101112- SISlag inclusion1:28–1:41 · 1.47" · d 0.02"SI exceeds API 1104 acceptance limits — charged for re-work.
- EUExcess reinforcement9:53–9:55 · 0.21" · d 0.06"Within acceptance limits.
Visual inspection (CWI)
API 1104
Coating inspection
No coating inspection recorded for this joint.