J-2720
repairRepair- Line
- LN-12
- Station
- 1632+00
- Weld date
- 2026-05-31
- Spec
- 24" × 0.375"
33.45920, -103.87320
No open cross-check alerts on this joint.
Welder passes
- RootWorking sideOdell Rains RC-121
May 31, 2026, 8:35 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- RootDitch sideDwayne Ferris RC-204
May 31, 2026, 8:35 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- Hot PassWorking sideTy Maldonado RC-552
May 31, 2026, 9:10 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- Hot PassDitch sideHector Ruiz RC-528
May 31, 2026, 9:10 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- FillWorking sideKelly Boudreaux RC-350
May 31, 2026, 9:45 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- FillDitch sideDale Whitcomb RC-533
May 31, 2026, 9:45 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- CapWorking sideSam Whitfield RC-388
May 31, 2026, 10:20 AM · logged by C. Ramirez (Survey)
WPS-1104-TI-11 Rev 1SMAW uphill 6G (fixed)E6010 / E7018-H4
4–36 in OD · wall 0.188–0.75 in · hardness 235 HV10 max
- CapDitch sideDale Whitcomb RC-533
May 31, 2026, 10:20 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
- RepairWorking sideDale Whitcomb RC-533
May 31, 2026, 10:30 AM · logged by C. Ramirez (Survey)
WPS-1104-DH-01 Rev 2SMAW downhill 5G / 6GE6010 / E8010-G
6–36 in OD · wall 0.188–0.75 in · hardness 248 HV10 max
NDT results
- RTRepair
May 31, 2026, 8:00 PM · D. Halloran (ASNT II)
Fit-up gap out of tolerance (charged to spread, not welder)
Not charged to a welder.
Repairable indication — grind and re-weld authorized.
RT film map — clock position2 indications12123456789101112- PORPorosity4:20–4:39 · 2.02" · d 0.05"POR exceeds API 1104 acceptance limits — charged for re-work.
- PORPorosity5:55–5:58 · 0.34" · d 0.06"Within acceptance limits.
Visual inspection (CWI)
API 1104
Coating inspection
No coating inspection recorded for this joint.